Dislocation densities of CMP processed sapphire wafers for GaN epitaxy

  • 발행 : 2003.05.01

초록

The sapphire wafers for blue light emitting devices were manufactured by the implementation of the surface machining technology based on micro-tribology. This process has been performed by grinding, lapping and polishing. The surfaces of sapphire wafers were mechanically affected by residual stress and surface default. This mechanical stress and strain can be cured by thermal anneal ing process. The sapphire crystalline wafers were annealed at $1100~1400^{\circ}C$ and then characterized by double crystal X-ray diffraction. The sample showed good quality of crystalline wafer surface wi th full width at hal f maximum of 16 arcsec for the 4-hour heat-treatment at $1300^{\circ}C$.