$WC-3%(Cr_3C_2)-2%(Mo_2C)-12%Ni$ carbides were ground with three different types of electroplated diamond wheels with respect to grain friability. The grinding ratio in the case of the highest toughness grains, A becomes the highest at the workpiece speeds of 40 and 70mm/min exhibiting larger effect with smaller workpiece speed. The grinding ratio with the medium toughness grain is higher than that of grain A at higher workpiece speeds than 100mm/min. The surface roughness becomes smaller with increasing the grain friability The increasing rate on surface roughness with the increase of workpiece speed becomes higher with using the grain of lower friability.