• Title/Summary/Keyword: 불균질

Search Result 421, Processing Time 0.016 seconds

Jangdo(Small Ornamental Knives) manufacturing process and restoration research using Odong Inlay application (오동상감(烏銅象嵌)기법을 활용한 장도(粧刀)의 제작기술 및 복원연구)

  • Yun, Yong Hyun;Cho, Nam Chul;Jeong, Yeong Sang;Jang, Chu Nam
    • Korean Journal of Heritage: History & Science
    • /
    • v.49 no.2
    • /
    • pp.172-189
    • /
    • 2016
  • In this research, literature research on the Odong material, mixture ratio, casting method and casting facility was conducted on contemporary documents, such as Cheongong Geamul. Also, a long sword was produced using the Odong inlay technique. The sword reproduction steps were as follows; Odong alloying, silver soldering alloying, Odong plate and Silver plate production, hilt and sheath production, metal frame and decorative elements, such as a Dugup (metal frame), production, Odong inlay assembly and final assembly. For the Odong alloy production, the mixture ratio of the true Odong, which has copper and gold ratio of 20:1, was used. This is traditional ratio for high quality product according to $17^{th}$ century metallurgy instruction manual. The silver soldering alloy was produced with silver and brass(Cu 7 : Zn 3) ratio of 5:1 for inlay purpose and 5:2 ratio for simple welding purpose. The true Odong alloy laminated with silver plate was used to produce hilt and sheath. The alloy went through annealing and forging steps to make it into 0.6 mm thick plate and its backing layer, which is a silver plate, had the matching thickness. After the two plates were adhered, the laminated plate went through annealing, forging, engraving, silver inlaying, shaping, silver welding, finishing and polishing steps. During the Odong colouring process, its red surface turns black by induced corrosion and different hues can be achieved depending on its quality. To accomplish the silver inlay Odong techniques, a Hanji saturated with thirty day old urine is wrapped around a hilt and sheath material, then it is left at warm room temperature for two to three hours. The Odong's surface will turn black when silver inlay remains unchanged. Various scientific analysis were conducted to study composition of recreated Odong panel, silver soldering, silver plate and the colouring agent on Odong's surface. The recreated Odong had average out at Cu 95.57 wt% Au 4.16wt% and Cu 98.04 wt% Au 1.95wt%, when documented ratio in the old record is Cu 95wt% and Au 5wt%. The recreated Odong was prone to surface breakage during manufacturing process unlike material made with composition ratio written in the old record. On the silver plate of the silver and Odong laminate, 100wt% Ag was detected and between the two layers Cu, Ag and Au were detected. This proves that the adhesion between the two layers was successfully achieved. The silver soldering had varied composition of Ag depending on the location. This shows uneven composition of the silver welding. A large quantities of S, that was not initially present, was detected on the surface of the black Odong. This indicates that presence of S has influence on Odong colour. Additional study on the chromaticity, additional chemical compounds and its restoration are needed for the further understanding of the origin of Odong colour. The result of Odong alloy testing and recreation, Odong silver inlay long sword production, scientific analysis of the Odong black colouring agent will form an important foundation of knowledge for conservation of Odong artifact.