Abstract
In this paper, we have designed the anti-reflection(AR) coating for $1400{\sim}1600$ nm wavelength range on the ferrule facet of optical connector. The low-temperature ion-assisted deposition was applied to AR coating on the ferrule facet in order to avoid damage of optical connector. We have measured the refractive index of coating film($Ta_2O_5\;and\;SiO_2$) using the ellipsometer and optimized the film thickness using the SEM and thickness measurement equipment. UV-VIS-NIR spectrophotometer is used to measure transmissivity of the AR coated ferrule facet. The refractive index of $Ta_2O_5\;and\;SiO_2$ is $2.123{\sim}2.125$ and $1.44{\sim}1.442$, respectively, for $1400{\sim}1600$ nm wavelength range. The transmissivity of the AR coated ferule facet is more than 99.8 % for $1425{\sim}1575$ nm wavelength range and more than 99.5 % for $1400{\sim}1600$ nm wavelength range. The return loss of the AR coated ferrule facet is 30.1 dB.