Melt-out Behaviour of 25wt% Al-Alloyed Ductile Iron

25wt% A1이 첨가된 구상흑연주철의 용손 거동

  • 권기현 (한국기계연구원 표면연구부) ;
  • 이종훈 (한국기계연구원 표면연구부) ;
  • 유위도 (한국기계연구원 표면연구부)
  • Published : 2004.12.30

Abstract

In this study, effect of temperature and time on melt-out of 25wt% Al-alloyed ductile iron has been investigated. The oxidation tests were carried out in a tube furnace at $800^\circC$, $930^\circC$, and $1000^\circC$ for lh, 5h, 10h, 50h. The microstructure, microhardness, and $Al_2O_3$ layer of oxidation-treated 25wt% Al-alloyed ductile iron samples (10 x 10 x 10 mm) were investigated. Phase identification was performed by X-ray diffraction(XRD) and EDS. The oxidation-treated 25wt% Al-alloyed ductile iron samples at $930^\circC$ for lh, 5h, 10h and KS GCD 500 were used for melt-out test in an Al alloy melt. The melt-out test results showed that oxidation tested sample at $930^\circC$ for 5h which on the whole forms $2-3\mum$ $Al_2O_3$ layer showed lowest melt-out depth. It was observed showed that appropriate Al203 layer can affect melt-out behaviors.

Keywords