Abstract
This study was to evaluate GMA welding characteristics of the A15083-O aluminum alloy according to the shield gas mixing ratio and heat input change. The GMA welding of the base metal was carried out with flour different shield gas mixing ratios(Ar100%+He0%, Ar67%+He33%, Ar50%+He50%, and Ar33%+He67%). Regarding the if1uence on the bead shape of the shield gas mixing ratio and heat input, the bead width was greatest in Ar100%+He0% mixture. But the penetration depth and area were greatest in Ar33%+He67% mixture considering that the lower Ax gas ratio, the higher bead depth and area. Also, dilution was also best in the shield gas mixing ratio. The size and number of deflects were least in Ar33%+He67% mixture. Higher He gas ratio resulted in less deflects detected by the radiographic inspection.