초록
Lamellar tearing susceptibility and through-thickness tensile ductility have been investigated in $40kg/mm^2 and 50kg/mm^2$ class tensile strength steel plates in terms of cleanliness of non-metallic inclusion and welding condition. The plate which had 0.01% cleanliness of A-type inclusion (MnS) had 61% of the reduction of area in the through-thickness direction and did not show lamellar tearing. Lamellar tearing susceptibility decreased with increasing the preheat and interpass temperature. The plate which had 0.04% cleanliness of A-type inclusion did not show lamellar tearing under the condition of 75.deg. C of preheat and interpass temperature.