U/RE Recovery Using Large-Scale LCC Electrowinning System

  • Published : 2018.05.31

Abstract

U/RE was electrochemically recovered to LCC at $50mA/cm^2$ from LiCl-KCl salt containing $0.5wt%UCl_3$, $0.22wt%NdCl_3$, 0.15wt%$CeCl_3$ and $0.07wt%LaCl_3$. The Cd in the LCC deposit was removed during the distillation using Cd distiller. U/RE product of 107g obtained from the distiller was installed to TG and then heated to $1200^{\circ}C$ to be consolidated. Dense U/RE metal ingot was not acquired through the consolidation process because U/RE product had been partially already oxidized during the distillation process.