Permittivity Properties of Titania-fused Silica

Titania-fused Silica의 유전특성 분석

  • 김한준 (한국표준과학연구원 전자기표준부 전기그룹) ;
  • 이래덕 (한국표준과학연구원 전자기표준부 전기그룹) ;
  • 시며노프 (러시아 VNIIM) ;
  • 한상옥 (충남대학교 전기공학과)
  • Published : 1999.07.19

Abstract

The thermal expansion coefficient of the titania-fused silica glass$(TiO_2-SiO_2)$ called KLR-1.1 is known to $0{\pm}0.03$ ppm/K, while that of normal fused-silica glasses is about +0.5 ppm/K at room temperature. To analysis the dielectric properties of the KLR-1.1, the sample with diameter of 30 mm and thinkness of 1 mm is covered with gold film. Its relative permittivity and dissipation factor of KLR-1.1 is evaluated to $4.011{\pm}0.012(1\sigma)$ and $(4.86{\pm}0.02){\times}10^{-4}(1{\sigma})$ at 1 kHz respectively. The measurement techniques used and results are more discussed in this paper.